Bearing Failure Analysis

Home/Products/Bearing Failure Analysis

Failure analysis

Read the damage. Find what started it.


A practical guide to 24 engine bearing damage examples, written for engine builders and counter staff. Each card shows what the damage looks like, the likely cause, and the fix.

How to use this page

The bearing acts like a fuse

A plain bearing often shows the problem first. When the oil, shaft, housing or assembly is at fault, the bearing is usually the part that records it. Read the damage, find the root cause, and fix that cause before you install new parts.

Daido sorts bearing damage into seven groups: scratching, wear, seizure, fatigue, corrosion, erosion and others. When several kinds of damage appear, find the one that started it. That is the real cause. Fatigue that later leads to scratching is still a fatigue problem.

Possible causes

Location alone is not a diagnosis; confirm with the full teardown.

Diagram of a Daido engine bearing half shell, inside view, with numbered markers for seven damage zones and an inset of the steel back
  1. Center load zone Fatigue from too much load; overlay fatigue in the loaded area when the shaft or housing is out of shape; seizure from shaft run-out; heavy scoring around the center from debris or burrs at the shaft oil hole; overlay worn off the loaded area by lead corrosion; suction cavitation in the land center.
  2. Edges Uneven contact from shaft or housing shape.
  3. Parting lines Overlay fatigue just inside both parting lines from heavy load and a shaft or housing that is out of shape; wear from uneven contact at the joint; fretting at the joint.
  4. Crush relief at the joint Fatigue from cap shift, with alloy worn away around the relief (lug side shown); impact cavitation near the inside relief from intermittent lubrication; debris embedded around the relief on the lug side, sometimes with seizure.
  5. Oil hole area Fatigue from bending: cracks on both sides of the oil hole where the shell is not supported over the housing oil hole; flow cavitation upstream of the oil hole; a large piece of metal embedded near the oil hole; darkening near the oil hole on the unloaded side from copper corrosion.
  6. About 45–60° from the joint Local contact about 45° from the joint, sometimes with deteriorated oil on the back; fatigue from the shell moving in the housing; crescent-shaped discharge cavitation about 60° from the joint from rapid movement of the shaft center.
  7. Steel back Fretting on the outside from minute vibration between the bearing and the housing; deteriorated oil stuck to the back behind a local contact; marks on the back from incorrect housing dimensions.

Some kinds of damage, such as fine scoring from lots of small debris, can cover the whole surface and do not have a single marker.

Damage examples

Recognize the damage. Find the cause.

Scratching

Score lines, spot scratches, and debris pressed into the surface.

Illustration of a bearing half-shell with heavy, irregular score lines in a band through the center of the running surface, while the top and bottom edges stay clean.

Example 1

Scoring through the center

Looks like: Heavy, irregular score lines in a band through the center of the bearing, sometimes cut through to the lining. The edges of the shell are often still clean.

Likely cause: Debris or a burr at the crankshaft oil hole, carried around with the journal.

Fix: Deburr the crank oil holes and clean every part thoroughly at assembly.

Illustration of a bearing half-shell with score lines and spot scratches over the whole running surface, from fine debris in the engine.

Example 2

Scoring over the whole surface

Looks like: Score lines and spot scratches over the whole running surface, not just the center.

Likely cause: A large amount of fine debris in the engine, often iron particles left from machining or assembly.

Fix: Clean every part thoroughly at assembly.

Illustration of a bearing half-shell with fine black carbon specks pressed into the overlay across the running surface.

Example 3

Embedded carbon

Looks like: Fine black specks pressed into the overlay across the surface, giving it a dark, dirty look.

Likely cause: Carbon from poor combustion and degraded oil.

Fix: Keep up oil and filter service, and address combustion problems.

Illustration of a bearing half-shell with a large metal fragment pressed into the running surface beside the oil hole, and a short drag trail.

Example 4

Embedded metal chips

Looks like: A larger chip or fragment pressed into the surface, often near the oil hole, sometimes with a short drag trail.

Likely cause: Metal left in the engine from machining or assembly.

Fix: Clean every part thoroughly at assembly.

Wear

Material worn away faster than it should be for the miles on the engine.

Illustration of a bearing half-shell with the overlay worn through unevenly, showing the lining underneath, with scoring and spot scratches from debris in the oil.

Example 6

Wear

Looks like: Overlay worn away unevenly, beyond normal wear for the miles, often with scratches from debris.

Likely cause: Abrasive debris in the oil, or uneven contact from journal or housing shape errors.

Fix: Clean the oil system, and check journal and bore geometry.

Seizure

The journal and bearing have made metal-to-metal contact and overheated.

Illustration of a bearing half-shell with the whole running surface smeared and heat-tinted after seizure, with dark debris near the parting line.

Example 5

Seizure from debris

Looks like: An overheated surface where bearing material has smeared, flowed or welded to the journal.

Likely cause: Metal-to-metal contact from lack of oil, start-up or shutdown, uneven contact, or heavy debris.

Fix: Restore oil supply and pressure, and clean the engine thoroughly.

Illustration of a main bearing half-shell with a seized, blackened band through the center of the running surface, typical of crankshaft run-out.

Example 7

Seizure from crankshaft run-out

Looks like: A seized, darkened band through the center of a main bearing, usually the center main.

Likely cause: A crankshaft that is bent or out of true pushes the journal hard into the middle bearings.

Fix: Check crankshaft run-out and journal precision before assembly.

Fatigue

Repeated load cracks the lining or the overlay until pieces flake out.

Illustration of a bearing half-shell with fatigue cracks running across the shell from both sides of the oil hole, caused by the shell flexing over the housing oil hole.

Example 8

Fatigue from bending

Looks like: Cracks running across the bearing from both sides of the oil hole.

Likely cause: The shell is not supported over a large or heavily chamfered housing oil hole, so it flexes there.

Fix: Check the size and chamfer of the housing oil hole, or review the bearing series for the duty.

Illustration of a bearing half-shell with lining flaked out in a strip next to the parting line, caused by cap shift.

Example 9

Fatigue from cap shift

Looks like: Lining flaked out in a strip next to the parting line.

Likely cause: A cap that has shifted puts extra load on the bearing near the parting line.

Fix: Check cap alignment, cap fit and dowels, and correct any cap shift.

Illustration of a bearing half-shell with a network of cracks and mosaic-shaped pieces of lining missing across the loaded area.

Example 10

Fatigue

Looks like: Cracks that join up until pieces of lining flake out like a mosaic, in the loaded area.

Likely cause: Load beyond what the bearing can carry, or journal and housing shape errors.

Fix: Reduce the load, correct shaft and housing geometry, or review the bearing series for the duty.

Illustration of a bearing half-shell with fine crazing and small pits in the overlay across the loaded center, with lining showing in spots.

Example 11

Overlay fatigue in the load zone

Looks like: Fine crazing and small pits in the overlay where the load acts, with lining showing through in spots.

Likely cause: Heavy load combined with a journal or housing that is out of shape.

Fix: Correct journal and housing shape, or review the bearing series for the duty.

Illustration of a bearing half-shell with crazed, pitted overlay in a strip just inside both parting lines, while the center stays clean.

Example 12

Overlay fatigue at the parting lines

Looks like: Fine crazing and pits in the overlay in a strip just inside both parting lines. The center of the shell is often still clean.

Likely cause: Heavy load plus a journal or housing that is out of shape, which overloads the bearing near the joints.

Fix: Correct journal and housing shape, or review the bearing series for the duty.

Illustration of a bearing half-shell with a local contact zone near one parting line, with fatigue cracks and flaking inside it.

Example 23

Fatigue from shell movement

Looks like: A local contact spot partway around from the parting line, with cracks and flaking inside it.

Likely cause: The shell moves in its housing because the bore is machined to the wrong size, overloading one spot on the face.

Fix: Confirm housing bore dimensions and crush, and check housing rigidity.

Corrosion

Degraded oil or high temperature attacks the lead or the copper in the lining.

Illustration of a bearing half-shell with a dull, darkened surface covered in pinholes across the loaded area from corrosion.

Example 13

Lead corrosion

Looks like: A dull, darkened, spongy-looking surface covered in pinholes, with the overlay gone over the loaded area.

Likely cause: Degraded oil and overdue changes attack the lead in the bearing.

Fix: Review oil quality and change intervals.

Illustration of a thrust washer face with a pitted, spongy alloy surface and only small patches of overlay left.

Example 14

Lead corrosion on a thrust face

Looks like: A pitted, spongy thrust face, with only small patches of overlay left.

Likely cause: Degraded oil and overdue changes attack the lead in the bearing.

Fix: Review oil quality and change intervals.

Illustration of a bearing half-shell with a large blackened area around the oil hole and a darkened load band from copper corrosion.

Example 15

Copper corrosion

Looks like: A large blackened area, often around the oil hole, with the load band darkened.

Likely cause: High oil and engine temperatures and degraded oil let copper in the lining react and form a dark film.

Fix: Check oil quantity and cooling, and review oil quality.

Erosion

Cavitation, fretting, and electrical pitting remove or frost the surface.

Illustration of a bearing half-shell with a band of cavitation erosion running around the center of the land through the oil hole.

Example 16

Suction cavitation

Looks like: A band of erosion running around the center of the bearing through the oil hole line.

Likely cause: Vapor bubbles collapsing on the surface when the journal moves rapidly in its clearance.

Fix: Review oil clearance, and raise oil pressure and supply.

Illustration of a bearing half-shell with a tear-shaped eroded area trailing from one side of the oil hole.

Example 17

Flow cavitation

Looks like: A tear-shaped eroded area trailing from one side of the oil hole.

Likely cause: Uneven oil flow at the oil hole.

Fix: Improve oil supply and pressure, and check the oil hole and its chamfer.

Illustration of a bearing half-shell with ragged eroded patches near the parting line at the end of the shell.

Example 18

Impact cavitation

Looks like: Ragged eroded patches near the parting line at the end of the shell.

Likely cause: Interrupted oil supply that lets the oil film break up and re-form.

Fix: Review oil clearance and the oil supply path to the bearing.

Illustration of a bearing half-shell with two crescent-shaped erosion marks set in from each parting line.

Example 19

Discharge cavitation

Looks like: Crescent-shaped erosion marks set in from each parting line.

Likely cause: Rapid journal movement in its clearance, often worse with abnormal combustion.

Fix: Review oil clearance and correct detonation or other combustion problems.

Illustration of a bearing half-shell with dark, frosted fretting patches on the running surface and no scoring.

Example 20

Fretting on the running surface

Looks like: Dark, frosted patches on the bearing face with no scoring.

Likely cause: Tiny vibration between bearing and journal while the engine is not running, often during shipping.

Fix: Support assembled engines properly in transport and reduce loads on the crank before shipping.

Illustration of the steel back of a bearing half-shell with frosted, oxide-stained fretting marks from movement between the shell and the housing.

Example 21

Fretting on the steel back

Looks like: Dark, frosted, oxide-stained marks on the steel back or joint faces.

Likely cause: Tiny movement between shell and housing from too little crush or a flexible housing.

Fix: Check housing bore size, crush and cap torque, and housing rigidity.

Illustration of a bearing half-shell with the whole running surface dull, dark and finely pitted from electrical current passing through it.

Example 24

Electrical erosion

Looks like: A dull, dark, finely pitted surface on the bearing, with the same marks on the journal.

Likely cause: Electrical current passing between the crankshaft and the block.

Fix: Check for electrical leakage and confirm ground connections.

Others

Damage from housing fit or debris behind the shell that does not fit the groups above.

Illustration of a bearing half-shell with one local rubbed-through mark on the running surface, caused by deposits trapped behind the steel back.

Example 22

Back-side contact problems

Looks like: A local rubbed spot on the face, with matching deposits or marks on the steel back behind it.

Likely cause: Debris or deposits trapped behind the shell, or a housing that lets the shell move.

Fix: Install shells clean and dry, and confirm housing dimensions and rigidity.

Illustrations are recreations, not photos of actual parts, with damage exaggerated for clarity. Real wear may be far subtler.

Resources

Tech resources and help

Materials, installation notes, the catalog, or a question for a bearing engineer.

Bearing Tech Info

How a plain bearing is built, what each series is made of, what we measure, and how to install it.

Open Tech Info

Catalog

Search by engine, part number or series, with the sizes available for each part.

Open Catalog

Cross Reference

Match Clevite, King, ACL, Sealed Power and Dura-Bond part numbers to Daido.

Open Cross Reference

Daido Technology

Multi-Boring, DE-LUG and the other Daido bearing design features.

See Technology

Ask a bearing engineer

Clearance, sizing or application questions. Email dmusa-ATC@daidometal.com or call (248) 893-2454.

Contact Us

Where to Buy

Daido engine bearings are sold through authorized distributors.

Find a Distributor